渗透等级

渗透式供给可用于为碎石路面提供冷沥青或热沥青。在这种类型的道路建设中,将使用薄层进行颅内开发,以保护下层免受潮湿的水和空气的影响,然后将其余的床层连接在一起,使路面更难铺设。

 

沥青渗透分析 40/50

Test TitleResultStandard rangeTEST Method
SP gr @25/25 cc1.04Min: 1.01 - Max: 1.06ISIRI 2956 - ASTM D70
Penetration @25c c-100gr-5s45.7Min: 1.01 - Max: 1.06ISIRI 2950 - ASTM D5
Softening Point 53.2Min: 1.01 - Max: 1.06ISIRI 3868 - ASTM D36
Solubility in Trichloroethylene (bitumen content)99.99Min: 1.01 - Max: ---ISIRI 2953 - ASTM D4
Ductility @25 cc cm>100 Min: 1.01 - Max: ---ISIRI 3866 - ASTM D113
Flash Point cc 319 Min: 1.01 - Max: ---ISIRI 1175 - ASTM D92
Loss On heating w t%0.03Min: --- - Max: 0.2ISIRI 2957 - ASTM D6
Drop Penetration after loss on heat8.1Min: --- - Max: 20ISIRI 2950 - ASTM D6 & D5
Spot TestNegativeNegativeISIRI 2949


沥青渗透分析 60/70

Test TitleResultStandard rangeTEST Method
SP gr @25/25 cc1.02Min: 1.01 - Max: 1.06ISIRI 2956 - ASTM D70
Penetration @25c c-100gr-5s65.4Min: 60 - Max: 70ISIRI 2950 - ASTM D5
Softening Point 49.7Min: 49 - Max: 56ISIRI 3868 - ASTM D36
Solubility in Trichloroethylene (bitumen content)99.99Min: 99.5 - Max: ---ISIRI 2953 - ASTM D4
Ductility @25 cc cm>100 Min: 100 - Max: ---ISIRI 3866 - ASTM D113
Flash Point cc 321Min: 232 - Max: ---ISIRI 1175 - ASTM D92
Loss On heating w t%20.0Min: --- - Max: 0.2ISIRI 2957 - ASTM D6
Drop Penetration after loss on heat38.Min: --- - Max: 20ISIRI 2950 - ASTM D6 & D5
Spot TestNegativeNegativeISIRI 2949


沥青渗透分析 85/100

Test TitleResultStandard rangeTEST Method
SP gr @25/25 cc1.02Min: 1.01 - Max: 1.06ISIRI 2956 - ASTM D70
Penetration @25c c-100gr-5s91.2Min: 85 - Max: 100ISIRI 2950 - ASTM D5
Softening Point 45.9Min: 45 - Max: 0ISIRI 3868 - ASTM D36
Solubility in Trichloroethylene (bitumen content)99.98Min: --- - Max: ---ISIRI 2953 - ASTM D4
Ductility @25 cc cm>100 Min: 100 - Max: ---ISIRI 3866 - ASTM D113
Flash Point cc 322Min: 232 - Max: ---ISIRI 1175 - ASTM D92
Loss On heating w t%0.03Min: --- - Max: 0.2ISIRI 2957 - ASTM D6
Drop Penetration after loss on heat8.1Min: --- - Max: 20ISIRI 2950 - ASTM D6 & D5
Spot TestNegativeNegativeISIRI 2949


沥青渗透分析 120/150

Test TitleResultStandard rangeTEST Method
SP gr @25/25 cc1.013Min: 1.01 - Max: 1.06ISIRI 2956 - ASTM D70
Penetration @25c c-100gr-5s132.0Min: 120 - Max: 150ISIRI 2950 - ASTM D5
Softening Point 42Min:38 - Max: 0ISIRI 3868 - ASTM D36
Solubility in Trichloroethylene (bitumen content)99.99Min: --- - Max: ---ISIRI 2953 - ASTM D4
Ductility @25 cc cm>100 Min: 100 - Max: ---ISIRI 3866 - ASTM D113
Flash Point cc 323Min: 232 - Max: ---ISIRI 1175 - ASTM D92
Loss On heating w t%0.03Min: --- - Max: 0.2ISIRI 2957 - ASTM D6
Drop Penetration after loss on heat8.3Min: --- - Max: 20ISIRI 2950 - ASTM D6 & D5
Spot TestNegativeNegativeISIRI 2949


沥青渗透分析 200/300

Test TitleResultStandard rangeTEST Method
SP gr @25/25 cc1.011Min: 1.01 - Max: 1.06ISIRI 2956 - ASTM D70
Penetration @25c c-100gr-5s250.0Min: 200 - Max: 300ISIRI 2950 - ASTM D5
Softening Point 38Min:35 - Max: 40ISIRI 3868 - ASTM D36
Solubility in Trichloroethylene (bitumen content)99.98Min: --- - Max: ---ISIRI 2953 - ASTM D4
Ductility @25 cc cm>100 Min: 100 - Max: ---ISIRI 3866 - ASTM D113
Flash Point cc 325Min: 232 - Max: ---ISIRI 1175 - ASTM D92
Loss On heating w t%0.04Min: --- - Max: 0.2ISIRI 2957 - ASTM D6
Drop Penetration after loss on heat8.2Min: --- - Max: 20ISIRI 2950 - ASTM D6 & D5
Spot TestNegativeNegativeISIRI 2949